Drone site insights · One Jump

Viaduct Inspection

2 viaducts4 flights354 photos4 min 4K videopreliminary
Preliminary results, 3 November 2026. The analysis is still running: every photo is being checked for defects (35 of 354 so far), Viaduct B's 3D model and the video's joint-by-joint record are in progress, and lengths in millimetres will be added to each defect. The numbers below come from the parts that are finished, and this page will be updated as the rest completes.

Two viaducts, flown from underneath

A small drone flew beneath two concrete viaducts with its camera tilted up at the underside. Viaduct A, an in-service box girder over housing, was flown on two consecutive days, once at 12 MP and once at 50 MP over the same stretch. Viaduct B, a long segmental viaduct, was photographed at 50 MP and filmed in 4K along about 0.8 km. Site names and locations are withheld.

28.8 m
Viaduct A span, pier centre to centre (±0.5 m)
97.7%
of Viaduct A's modelled underside seen in at least one photo
0.45–1.1 mm
finest pixel on the concrete (median per face)
≈ 250 m²
of Viaduct A underside measured from the 3D model
23
observations accepted after review by eye (63 rejected)
2.4×
finer detail at 50 MP than 12 MP on the same concrete
13 min
for 192 under-deck photos of one Viaduct A span
0.8 km
of Viaduct B recorded in a 4-minute 4K video

The underside area is the bottom flange (78.5 m²), both webs (90.1 m²) and the cantilever undersides (77.9 m²), measured from the underside passes (Viaduct A section below). Uncertainties are one standard deviation.

What the flights tell an owner, a contractor and an inspector

Each insight says what the data shows, why it matters, who uses it and what to do next. Inspection-practice references are to published Australian state road agency manuals (listed under Sources); a formal condition rating remains the job of an accredited bridge inspector on site.

Asset registerViaduct A

Element quantities in the units inspectors record

Shows
One 28.8 m (±0.5 m) span between two circular piers about 1.5–1.6 m across. The box girder's bottom flange is 2.86 m wide (±0.06 m) with webs 1.33 m and 1.08 m deep on the two sides and a 4.4% cross-fall. Measured concrete faces: bottom flange 78.5 m² (±4.9), both webs 90.1 m² (±5.6), cantilever undersides 77.9 m² (±4.8), one side face 134 m² (±8).
Why
Australian manuals record box girders, piers and headstocks by quantity, and one state manual records them as square metres of exposed surface so that maintenance quantities and costs can be estimated across a network. Condition is split across states 1–4 as shares of those quantities.
Who
Asset owner and maintainer (asset register, where drawings are missing or out of date); maintenance contractor (scoping).
Next
Use these areas as the denominators for the condition split per element; check them against drawings where they exist.
CoverageViaduct A

A re-fly list before the crew leaves site

Shows
97.7% of the 203 m² underside plan in the 3D model was seen in at least one photo, almost all of it by the 27 August flight (97.6%, and 93.7% by three or more photos). One side face was covered 99.7%, the other 87.3%. The gaps are small patches near the pier ends and along one web edge (red on the coverage map).
Why
A detailed (Level 2) inspection expects every component looked at from within about 3 m or an equivalent view, and an element with a quarter or less visible has to be reported as an exception. A coverage map turns "did we see everything?" into a list of spots.
Who
Drone operator and inspector on the day; asset owner auditing what was inspected.
Next
Compute the map on site after the flight and re-fly the red patches before demobilising.
CracksViaduct Apreliminary

Which crack widths this camera can and cannot rate

Shows
The finest pixel on the concrete was 0.45 mm on the closest side face, 0.9 mm on the underside and 1.06 mm on the far side face (median per face). Six fine lines consistent with hairline cracks were found and accepted by eye; four of them could also be scratches or form-panel marks, and one has light brown staining along it.
Why
The manuals band crack widths at 0.1, 0.3 and 0.6 or 0.7 mm. A crack narrower than a pixel can still show as a line, but its width cannot be measured, so from these photos the cracks can be located and counted but not yet placed in a width band.
Who
Inspector (where to put the crack gauge); owner (which cracks need a closer look).
Next
Revisit the flagged lines with 50 MP close passes or a hands-on check with a crack gauge or scale target in the frame, as one of the manuals asks; record length, orientation and distance to the nearest support for each.
Water pathsViaduct Apreliminary

Where water is getting through

Shows
Six dark streaks running down vertical formwork joints, two water-stained areas (one brown-toned patch on the underside near the haunch), four dark staining patches and one fine crack with brown staining along it.
Why
Staining and leaching mark the path of water through or over the concrete; rust-coloured staining is an early sign of reinforcement corrosion, which later cracks, spalls and exposes the bars. Finding the water path early is the cheap fix.
Who
Maintainer (drainage and joint maintenance); owner (prioritising closer inspection).
Next
Check the drainage and joints above each streak; give the brown-toned patch and the stained crack a close look first.
Capture settingsViaduct A

12 MP for coverage, 50 MP where width matters

Shows
On the same concrete, the 50 MP photos hold 2.4 times as many pixels per metre (2.26–2.40 across matched pairs), so a 0.9 mm pixel becomes about 0.4 mm. Each 50 MP photo is 14.0 MB against 6.7 MB, and the camera took one every 5 s against every 2 s (12 against 30 photos per minute).
Why
Flight time and storage are set by photo count; resolution sets what can be rated. In the comparison, a paint mark's overspray speckle only resolves at 50 MP.
Who
Drone operator (mission planning); inspector (data that can be rated).
Next
Fly full-coverage passes at 12 MP, then targeted 50 MP passes over the flagged spots and the zones where cracks matter most (near supports and at midspan).
Image qualityViaduct Apreliminary

Under a deck, hold still for each photo

Shows
Of 30 side-face photos at 12 MP checked so far, 13 were flagged and 5 are worth re-taking: the aircraft was still moving at 1/80–1/120 s shutter, giving an estimated 3–6 pixels of smear. Image noise at ISO 200–280 was low.
Why
Shade under the deck pushes the camera to slow shutter speeds, and smear hides exactly the fine lines an inspection is looking for. The low noise means there is room to raise ISO for a faster shutter.
Who
Drone operator.
Next
Set a faster minimum shutter speed under decks and pause for each shot; check sharpness on site and re-take the flagged frames.
Repeat inspectionViaduct Apreliminary

A record that can be compared next time

Shows
Photos from 27 and 28 August were matched to each other automatically, and the same staining patch and pier head were found on both days. The full day-to-day comparison waits for every photo to be checked (only 3 photos from 27 August were in the first batch).
Why
Condition profiles from repeated inspections feed deterioration models and maintenance budgets. A dated, matched record answers "was it there last time, and has it grown?" without a person standing at the same spot.
Who
Owner and maintainer (trend), insurer (evidence of condition at a date), contractor (defects liability).
Next
Re-fly the same passes at the next inspection and compare defect by defect.
HousekeepingViaduct A

Cosmetic items and what the photos cannot reach

Shows
Three paint marks (graffiti remnants) and bird droppings at a pier top. Wire-mesh enclosures on the pier tops hide the bearings.
Why
Cleaning and graffiti removal are routine maintenance line items; bearings need their own close inspection.
Who
Maintainer.
Next
Add the marks to the cleaning programme; schedule a bearing check from the pier cap.
Handover baselineViaduct Bin progress

Every segment joint on record

Shows
92 photos at 50 MP from beneath and beside the structure, and a 4-minute 4K video along about 813 m of it, flown at a median 24 m above take-off and 13 m/s in the long passes. The precast segment joints are visible along the girder's side; a joint-by-joint record is being built.
Why
One published manual asks for a detailed inspection before handover and again four months before the defects liability period ends, so the builder can fix construction defects. A dated photo of every joint settles "was it there at handover?". (This is the use case; we make no claim about this structure's contract.)
Who
Construction contractor, owner's representative, future maintainer.
Next
Repeat the same flight before the end of the defects liability period and compare joint by joint.
Access and method

What published studies say about time and cost

Shows
On Viaduct A, a 13-minute flight covered one span's underside in 192 photos.
Why
A US national study (NCHRP Research Report 1114, 2024) timed a multi-box-girder approach span at 30–60 minutes from an aerial lift or the ground and about 15 minutes per span by drone, both seeing only the outside of the boxes. An Oregon DOT study (2018) estimated a saving of about USD 10,200 per suitable bridge in staff, equipment and traffic control, with significant uncertainty. We found no published Australian figures, so these are context, not a forecast for these viaducts.
Who
Owner and inspection consultant (method selection).
Next
Record time on site, access equipment and closures avoided on each flight so the comparison can be made with local numbers.

Viaduct A: the underside, mapped

192 under-deck photos (27 August, 13 minutes) were turned into a 3D model and scaled with the drone's GPS and barometer (scale uncertainty 1.6%). Below, the underside of the span is drawn as a reflected plan, as if looking down through the deck.

Reflected plan of the box girder underside: flat bottom flange with panel joints, inclined webs and cantilever undersides
Underside of one span, 0.01 m per pixel. The flat strip is the bottom flange; panel joints run across it every few metres.
Coverage map of the underside: mostly amber, with small red gaps near the pier ends and along one web edge
seen in 1 flight2 flights3 flightsnot seen
Same view: which flights saw each 5 cm cell. The red patches are the re-fly list.
Side elevation of the girder web and deck edge along the span
One side face along the span, from the side passes.
MeasurementValue±1σHow
Span, pier centre to centre28.81 m0.46 mCircle fits to the pier tops; 28.84 m from the other flights
Pier diameter just below the top enclosure1.51–1.59 m0.05–0.06 mOnly the top 0.5–1 m of each pier is in the photos
Bottom flange width2.86 m0.06 mMedian of 53 cross-sections, 0.5 m apart
Web depth, side 1 / side 21.33 / 1.08 m0.03 / 0.02 mSame cross-sections
Bottom cross-fall4.4%0.15%Same cross-sections
Longitudinal gradient of the underside1.5%0.5%Line through the bottom flange
Underside height above the take-off point5.08 m0.17 mMedian; lowest 4.86 m near one pier. Measured from the take-off spot, not surveyed ground
Bottom flange area imaged78.5 m²4.9 m²Sum of the 3D model's surface on each face
Both webs, from below90.1 m²5.6 m²
Cantilever undersides, both sides77.9 m²4.8 m²
One side face (web and cantilever)134.1 m²8.3 m²

Defect register so far

Viaduct A only, from the first 35 photos checked. Image analysis flagged 185 candidate spots, grouped into 94 after removing repeats across photos; each was reviewed by eye, and 23 were accepted (2 of them spotted by eye rather than flagged). Formwork lines, panel joints and shadows were rejected. Labels say "consistent with" because a photo cannot confirm the cause.

IDPhotoTypeWhat was seenNoteSeen
A-01Patchy dark staining on the side faceDark stainingPatchy dark staining on the side faceAppears superficial27 & 28 Aug, both resolutions
A-02Dark sprayed stroke with a pale curved mark below itPaint markDark sprayed stroke with a pale curved mark below; overspray resolved at 50 MPConsistent with a graffiti remnant; cosmetic28 Aug, both resolutions
A-03–Pier headTop of a circular pier inside a wire-mesh enclosureNo defect visible; bearings hidden by the mesh27 & 28 Aug
A-04Dark streak down a vertical formwork jointJoint stainingDark streak down a vertical formwork jointAppears to be water tracking down the joint; check the joint above28 Aug, 12 MP
A-05Dark blotch below the drip lineDark stainingDark blotch below the drip lineAppears superficial; no loss of concrete visible28 Aug, 12 MP
A-06Dark mottled patch on the side faceDark stainingDark mottled patch on the side faceAppears superficial28 Aug, both resolutions
A-07Dark streak along a vertical formwork jointJoint stainingDark streak along a vertical formwork jointAppears to be water tracking down the joint28 Aug, 12 MP
A-08Dark streak along a vertical formwork jointJoint stainingDark streak along a vertical formwork jointAppears to be water tracking down the joint28 Aug, 12 MP
A-09Small dark smudge with fine scratchesPaint markSmall dark smudge with fine scratches, no depth or shadowConsistent with a paint or dirt mark, not spalling28 Aug, 12 MP
A-10Small hook-shaped dark markPaint markSmall hook-shaped dark mark with a faint pale stroke, no shadow or depthConsistent with a paint or dirt mark; spotted by eye28 Aug, 12 MP
A-11Fine dark diagonal line crossing the side faceHairline crack?Fine dark diagonal line crossing the side faceConsistent with a hairline crack, could be a scratch; width below what 12 MP resolves28 Aug, 12 MP
A-12Fine dark diagonal line running to the bottom edgeHairline crack?Fine dark diagonal line running to the bottom edgeConsistent with a hairline crack, could be a scratch28 Aug, 12 MP
A-13Fine dark line on the side faceHairline crack?Fine dark diagonal line on the side faceConsistent with a hairline crack, could be a scratch; width below what 12 MP resolves28 Aug, 12 MP
A-14Long fine diagonal line with a slight step along itHairline crack?Long fine diagonal line with a slight step along itConsistent with a hairline crack or a form-panel mark; confirm closer28 Aug, 12 MP
A-15Dark streak along a vertical formwork jointJoint stainingDark streak along a vertical formwork jointAppears to be water tracking down the joint28 Aug, 50 MP
A-16Dark blotch below the horizontal drip lineDark stainingDark blotch below the horizontal drip lineAppears superficial28 Aug, 50 MP
A-17Vertical streak of dark spots along a formwork jointJoint stainingVertical streak of dark spots along a formwork jointConsistent with water tracking down the joint28 Aug, 50 MP
A-18Dark streak down a vertical formwork joint to the deck edgeJoint stainingDark streak down a vertical formwork joint to the deck edgeAppears to be water tracking down the joint27 Aug
A-19–Bird foulingWhite streaks down the pier top below the wire-mesh enclosureConsistent with bird droppings; bearings not clearly visible27 Aug
A-20Fine wavy vertical lines with light brown staining along themFine crackingFine wavy vertical lines with light brown staining along themSuggests moisture passing through, possibly with some rust; check at close range27 Aug
A-21Thin dark curved line from a panel joint with hand-drawn strokes beside itHairline crackThin dark curved line from an underside panel joint; white and faint red hand-drawn strokes beside itThe strokes look like marking from an earlier inspection27 Aug
A-22Brown-toned stain spreading across the underside near the haunchWater stainingBrown-toned stain spreading across the underside near the haunchConsistent with water staining, possibly carrying rust or dirt; check the source above27 Aug
A-23Dark vertical streak on the faceWater stainingDark vertical streak on the faceConsistent with water run-off; cosmetic27 Aug

"Seen" lists the photo sets checked so far in which the item was found; sets not yet checked may show it too.

Capture settings: 12 MP against 50 MP

On 28 August the same stretch of Viaduct A was flown twice, minutes apart. Each pair below shows the same patch of concrete: 12 MP on the left, 50 MP on the right.

Paint mark at 12 MP and at 50 MP side by side
A-02 paint mark: the overspray speckle only resolves at 50 MP.
Dark staining at 12 MP and at 50 MP side by side
A-01 staining: edges and texture sharpen at 50 MP.
Mottled staining at 12 MP and at 50 MP side by side
A-06 mottled staining at both resolutions.
12 MP50 MP
Image size4096 × 23048192 × 4608
Pixels per metre on the same concrete1×2.38× (2.26–2.40)
Average file size6.7 MB14.0 MB
Time between photos2 s5 s
Photos per minute3012
Data written per minute198 MB170 MB
Photos in this comparison45 in 88 s25 in 120 s

Viaduct B: a long segmental viaduct

A 4K video flown along the structure and 92 photos at 50 MP from beneath and beside it (23 August, about 20 minutes for the photos). The 3D model, the segment-joint record and stored joint and pier boxes for the video are in progress.

10 s from the 4-minute video. The vertical lines along the girder's side are the joints between precast segments.

From the video's flight record

Video length4 min 11 s
Distance along the viaduct≈ 813 m (GPS ±2 m)
Height above take-off, long passesmedian 23.6 m (max 34.1 m)
Speed, long passesmedian 13.4 m/s (max 15.3)
Camera angle, long passes15–19° below horizontal
Photos92 × 50 MP, camera −28° to +46°

At 13 m/s the video records the structure in minutes but from further away than the photos; the photos are the close-range record. Both feed the joint-by-joint baseline.

What this data cannot show

  • Crack widths narrower than about one pixel cannot be measured; such a crack may still show as a faint line.
  • Only surfaces the camera saw: the inside of the box girders, the top of the deck, the far faces and anything behind the pier-top enclosures were not photographed.
  • Bearings are not visible in these photos and need a close look from the pier cap.
  • Delamination without a visible surface change (hollow concrete) needs tapping or thermal imaging.
  • Colour alone cannot tell rust staining from iron-rich dirt, or white deposits from paint or droppings; labels say "appears" or "consistent with".
  • No laser range finder and no RTK positioning: distances come from the 3D model scaled by GPS and barometer, and GPS under a deck is degraded. A known target in a few photos would tighten the scale.

Sources

Accessed 3 November 2026. Inspection practice is paraphrased; US figures are quoted as published and are not forecasts for these structures.

The figures on this page as data: data.json.